ENGAGE THE BEAST 3DFind my failure

Elegoo Centauri Carbon settings that work

Updated

Start from Elegoo's own OrcaSlicer profiles: pick "Elegoo Centauri Carbon" as the printer and the profile that matches your spool. The numbers below are what those profiles set. The Centauri Carbon is a CoreXY printer with a 256 × 256 × 256 mm build volume and a hardened steel nozzle.

Starting settings by filament

Nozzle temperature with the spool's allowed range in brackets, bed temperature across plate types, part cooling fan, and the fastest the profile lets plastic flow.

FilamentNozzleBedFanMax flow
Elegoo PLA220 °C (190–240)35–60 °C50–100%30 mm³/s
Elegoo PLA Matte220 °C (190–240)35–65 °C60–80%30 mm³/s
Elegoo PETG250 °C (230–270)70 °C10–40%11 mm³/s
Elegoo PETG PRO240 °C (230–270)70 °C10–40%21 mm³/s
Elegoo ABS270 °C (240–280)90 °C10–40%18 mm³/s
Elegoo ASA270 °C (240–280)90 °C10–80%30 mm³/s
Elegoo PLA-CF220 °C (190–240)45–65 °C60–80%16 mm³/s
Elegoo PETG-CF250 °C (240–270)70 °C5–40%15 mm³/s
Elegoo PAHT-CF290 °C (260–290)35–100 °C10–30%8 mm³/s
Elegoo TPU 95A225 °C (200–250)30–35 °C100%3.2 mm³/s

Another brand of filament? MakerBeast has 961 filament profiles and checks the settings against your printer. Open MakerBeast.

Common Centauri Carbon problems and fixes

Stringing / whiskers

Fine hairs or cobwebs between separate parts of the print.

Usual causes, most likely first

  1. Wet filament: water boils in the nozzle and keeps pushing plastic out (PETG, nylon and TPU especially).
  2. Nozzle too hot for that filament.
  3. Retraction too short or too slow for your extruder.
  4. Travel moves crossing open air instead of staying inside the part.

Fixes, in order

  1. Dry the spool, then print the same file again. If the strings shrink, moisture was the cause.
  2. Lower the nozzle 5 °C at a time, staying inside the spool's range.
  3. Run the retraction test in your slicer's Calibration menu.
  4. Turn on 'Avoid crossing walls' (OrcaSlicer, Bambu Studio) or 'Combing' (Cura).

A quick check: if you hear popping or see steam at the nozzle, the filament is wet.

Diagnose my stringing problem →

Corners lifting / warping

Corners peel up off the bed; the bottom of the part curves.

Usual causes, most likely first

  1. Plastic shrinks as it cools and pulls the corners up. ABS, ASA, nylon and PC shrink the most.
  2. Drafts or cold room air, or an open enclosure.
  3. Bed too cool, or a dirty plate (fingerprints are enough).
  4. Part cooling fan too high for that material.

Fixes, in order

  1. Wash the plate with dish soap and hot water, then don't touch the print surface.
  2. Use a brim (5–8 mm) on parts with sharp corners.
  3. Keep the enclosure closed and let the bed heat the chamber for 10–15 minutes before printing ABS/ASA/PC.
  4. Lower part cooling for shrink-prone materials.

Rounded corners in your design warp far less than sharp ones.

Diagnose my corners lifting problem →

Won't stick to the bed

The first layer drags around, curls up, or never sticks at all.

Usual causes, most likely first

  1. Nozzle too far from the bed (first layer is round beads, not flattened lines).
  2. Oily or dusty plate.
  3. Bed too cool for the material.
  4. First layer printing too fast.

Fixes, in order

  1. Clean the plate with dish soap and hot water. Isopropyl alcohol alone only moves oil around.
  2. Re-run bed leveling, then adjust Z-offset until the first layer lines are slightly flattened and touching.
  3. Use the bed temperature from the spool label.
  4. Slow the first layer to about 30–50 mm/s.

Diagnose my won't stick to the bed problem →

More failures and fixes are in the 3D print failure library.

Questions

What are good starting settings for the Elegoo Centauri Carbon?

Pick "Elegoo Centauri Carbon" as the printer in OrcaSlicer and the filament profile that matches your spool. For Elegoo PLA that profile sets the nozzle to 220 °C, and for Elegoo PETG 250 °C; the table on this page lists the rest.

Can the Centauri Carbon print carbon-fiber filaments?

Its profile lists a hardened steel nozzle, which is what abrasive carbon- and glass-fiber filaments need. Elegoo's own PLA-CF, PETG-CF and PAHT-CF profiles are in the table.

Why is my Centauri Carbon print stringing or warping?

Stringing is most often wet filament; warping is most often a dirty plate or drafts. The fixes are below, and MakerBeast's Failure Finder can name the cause from photos of the print and its G-code.

Can I watch my Centauri Carbon from my phone?

Yes. The MakerBeast phone app works with the Centauri Carbon. It needs Beast Bridge on a computer or an old Android phone on your Wi-Fi.